PSI - Issue 2_A
S Choudhury et al. / Procedia Structural Integrity 2 (2016) 736–743 S. Choudhury, S. K. Acharyya, S. Dhar/ Structural Integrity Procedia 00 (2016) 000–000
741
6
4.2 Estimation of G fr from the slope of J m-pl versus Δ a Curve
0 100 200 300 400 500 600 700 800 900
0 100 200 300 400 500 600 700 800
y = 307.2x + 444.0
y = 336.9x + 336.9
Serie1 Lineare (Serie1)
Serie1 Lineare (Serie1)
JM‐pl(N/mm2)
0,000
0,500
1,000
1,500
0
0,5
1
Crack Growth (mm)
Fig 5. J M-pl versus Crack growth at 22°C
Fig 6. J M-pl versus Crack growth at 0°C
0 100 200 300 400 500 600 700 800
0 100 200 300 400 500 600 700 800
y = 323.0x + 393.1
y = 310,05x + 349,75
2 )
Serie1
Lineare (Serie1)
J M‐pl (N/mm
Serie1 Lineare (Serie1)
JM‐pl (N/mm2)
0
0,5
1
1,5
0
0,5
1
Crack Growth (mm)
Crack Growth (mm)
Fig 7. J M-pl versus Crack growth at -20°C
Fig 8. J M-pl versus Crack growth at -40°C
0 100 200 300 400 500 600 700 800
0 100 200 300 400 500 600 700 800
y = 295.9x + 327.5
y = 209.8x + 521.7
Serie1 Lineare (Serie1)
Serie1 Lineare (Serie1)
JM‐pl (N/mm2)
JM‐pl (N/mm2)
0
0,5
1
1,5
0,00
0,50
1,00
1,50
Crack Growth (mm)
Crack Growth (mm)
Fig 9. J M-pl versus Crack growth at -60°C
Fig 10. J M-pl versus Crack growth at-7 0°C
Made with FlippingBook. PDF to flipbook with ease