PSI - Issue 13
Dan Eliezer et al. / Procedia Structural Integrity 13 (2018) 2233–2238 Eliezer et al/ Structural Integrity Procedia 00 (2018) 000 – 000
2236
4
DSS. At this lower dynamic pressure hydrogen has enough time to propagate a crack. This demonstration clearly represents the HAC phenomenon; when hydrogen is presented in a bulk metal it will promote cracking.
(b)
(c)
(a)
Non-charged
DSS SMSS AUSS
H charged
1000
800
600
400
Yield Strength [MPa]
30 MPa H 2 pressure
200
20 μm
20 μm
5 10 15 20 25 30 35 40 45 50 55
Elongation [%]
Fig. 3. (a) Quasi-static tensile test results of gas-phase charged DSS, SMSS and AUSS, and microstructural observations of cross-sectioned dynamic loaded hydrogen charged DSS: (b) non-charged and (c) hydrogen charged.
2.3. The effect of hydrogen-induced second phase on hydrogen trapping mechanism
The hydrogen trapping mechanisms were analyzed using thermal desorption analysis (TDA).The hydrogen evolution rate as a thermally activated process from trap sites were given by Lee and Lee's model [22]: / = ( − ) (− / ), (2) where X is the hydrogen content that escapes a trap, A is the reaction rate constant, E a is the activation energy for releasing hydrogen from its trapping site, R is the gas constant, T c is the peak of the absolute temperature and φ is the heating rate. The trap activation energy is measured from the linear relation [22]: ( / )/ ( / ) = − / , (3) A Peak position is related to a suitable activation energy; higher temperatures indicates higher binding energies, Fig. 4 [2].
Fig. 4. TDS spectra at a 6 o C/min heating rate of 72 h cathodic hydrogen charged samples: SMSS, DSS, and AUSS.
The -martensite phase trapping site appears only in SMSS and DSS where the -phase stability is lower and the