PSI - Issue 12

Massimiliano Avalle et al. / Procedia Structural Integrity 12 (2018) 19–31 Massimiliano Avalle / Structural Integrity Procedia 00 (2018) 000 – 000

22

4

 f P ( ρ ) density function for the plateau stress level  f S ( ρ ) density function for the intermediate phase  f D ( ρ ) density function for the densification parameter

In this way, the influence of the density is also included in the formulation. In most cases a power law approximation is a good description of the influence of the density. The proposed model fits very well the mechanical behavior of several foams in various loading conditions and at different densities. In the following sections the identification of the parameters for such materials, from experimental tests previously performed by the authors, are reported and discussed. There are situations where it is necessary to describe the loading of the foam after previous compression at a certain level, or to analyze repeated loading at different values. Since the foam behavior is highly non-linear, the behavior of the foam when loading from a strain different from the initial state is not easy to describe. Fig. 1 shows a typical situation: loading is non-linear up to a certain degree described by Eq. (6), unloading is equally non-linear following a different stress-strain relation, and leading to a residual strain; following re-loading is still non-linear following a relation similar to Eq. (3) but with different initial slope. Finally, it is known that, in each reloading, after a transition, the material tends to follow the basic characteristic as if loading-unloading has not occurred: the following reloading curves, as it is clear from Fig. 1 in light blue and green, all are overlapped to the curve corresponding to the normal loading path (curve in dark blue).

Stress, σ

ε 2

ε 1

Strain, ε

ε 0 = 0

ε 0,1 > 0

ε 0,2 > ε 0,1

Fig. 1. Description of the loading-unloading mechanisms.

From the analysis of several experimental tests, and based on the recognized expression (3) for the loading of the foam, it appears that repeated loading can be expressed as:

   

   

   

   

i 0,  

(6)

 

n     1 exp

      1 exp     m

r

i 

 

p

i

s

D

loading ,

0,

i

0,

With ε 0, i being the value of initial strain at the i -th reloading, that is the residual strain after the previous unloading. The new parameter r accounts for the observed reduction in the initial stiffness when reloading. It is important to note that the three parameters σ p plateau stress level, σ s linear hardening slope, σ D densification parameter and the m linear plateau transition coefficient and n Rusch densification exponent do not change in any reloading. Unloading is even more complex, especially because the curve parameters can change during each unloading.