PSI - Issue 64
Mao Ye et al. / Procedia Structural Integrity 64 (2024) 1824–1831 Author name / Structural Integrity Procedia 00 (2019) 000 – 000
1828
5
800
4% 6% 8% 10% 12% 16%
E 0
600
400
Stress plateau
Stress (MPa)
200
0 2 4 6 8 1012141618 0
Strain (%)
(a)
(b)
Fig. 3. (a) Stress-strain behavior of tensile specimen T-1; (b) Stress-strain behavior of prestraining specimens (No.1, 4, 5, 9, 12, and 13).
Table 2. Test results of prestraining, activation and re-activation.
Test type
Specimen No.
Prestrain level ε pre (%)
Elastic modulus E 0 (GPa)
Maximum tension stress σ max (MPa)
Residual strain ε res (%)
Activation temperature T act (℃) a
Recovery stress σ recov (MPa)
Prestraining & Activation
1 2 3 4 5 6 7
4
68.2 68.3 69.0 68.4 67.1 66.7 62.7 65.5 62.8 64.5 67.4 67.5 65.1 71.5 64.7 69.1 63.2 65.3
587.3 588.0 586.9 612.5 630.5 639.5 603.5 616.8 660.5 678.3 693.0 694.7 778.3 778.2 786.8 703.6 655.4 666.8
2.31 2.26 2.36 3.85 5.65 5.61 5.75 5.59 7.44 7.42 7.22 9.03
120 180 240 180 120 180 240 300 180 180 180 180 120 180 240
295.9 344.9 343.9 375.3 341.0 448.6 438.4 410.9 409.2 428.2 408.0 375.3 273.2 330.8 380.4
6 8
8 b 9 c
10
10 d 11 e
12 13 14 15 16 17 18
12 16
12.63 12.65 12.64
Prestraining & Activation & Re activation
10
7.43 7.43 7.43
120→180 180→240 240→240
355.2 → 418.0 414.2 → 443.2 440.9 → 445.0
Average 66.4 a For most activation tests, the average heating rate of each specimen was between 12~24 ℃ per minute.