Milivoje Jovanović et al. / Procedia Structural Integrity 31 (2021) 38 –44 M. Jovanovi ć et. al. / Structural Integrity Procedia 00 (2019) 000–000
41
4
Table 6. Impact test results for specimens with V-2 notch in HAZ
Impact total energy, AT, J
Crack initiation energy, AI, J
Crack propagation energy, AP, J
Specimen mark
HAZ - 1 HAZ - 2 HAZ - 3
248 246 249
70 59 70
178 187 179
Fig. 4. Impact test diagrams, for specimen HAZ-1
Table 7. Calculated values of K Ic for specimens notched in BM Specimen mark Testing temperature, C
Critical J-integral, J Ic , kJ/m 2
Critical stress intensity factor, K Ic , MPa m 1/2
PM-1K PM-2K PM-3K
131.1 144.2 124.0
173.9 182.4 169.2
20
Table 8. Calculated values of K Ic for specimens notched in WM Specimen mark Testing temperature, C
Critical J-integral, J Ic , kJ/m2
Critical stress intensity factor, K Ic , MPa m1/2
WM-1K WM-2K WM-3K
71.6 64.8 69.2
128.5 122.3 126.4
20
Figure 5. Diagrammes F- (a) and J- a (b) for the specimen PM – 1K