V. Yu. Filin et al. / Procedia Structural Integrity 28 (2020) 3–10 Filin V.Yu., Ilyin A.V.,Mizetsky A.V. / Procedia Structural Integrity 00 (2020) 000 – 000

9

7

Figure 4 – An example of simulated  m /  i distribution in fracture (1/2 fracture surface is shown).

a b Figure 5 – Simulated load-displacement curves: (a) at the same cleavage fracture criterion  = 2.7, (b) at the same coefficient  = 1.3. 4. Results of mechanical testing A steel rolled plate in the grade F40SW, 40 mm in thickness, was subjected to TKDS test. Table below gives a summary of the results. So for the metal of this plate TKDS temperature comes to -45°C. Temperature, °C Average ductile portion, % Average load drop, % -20 100 0 -30 90 13 -40 86 15 -50 70 40 -60 62 59 -90 21 97