E. Tsetsekou et al. / Procedia Structural Integrity 10 (2018) 227–234 E. Tsetsekou et al. / Structural Integrity Procedia 00 (2018) 00 – 000
231 5
MaximumLoad at Break - Controls
14000
12000
10000
Fir Maple
8000
6000
Load (N)
4000
2000
0
Casein
Fish Glue
Vinavil
Rabbit Glue Para loid B72
Fig. 4. The maximum load at break point of the five adhesives applied on fir and maple samples before ageing. All values are average of four replicates.
MaximumLoad at Break - UV
12000
10000
8000
Fir Maple
6000
4000 Load (N)
2000
0
Casein
Fish Glue
Vinavil
Rabbit Glue Para loid B72
Fig. 5. The maximum load at break point of the five adhesives applied on fir and maple samples after accelerating ageing with UV. All values are average of four replicates.
Maximum Load at Break - RH-T
0 1000 2000 3000 4000 5000 6000 7000 8000 9000 10000
Fir Maple
Load (N)
Casein Fish Glue Vinavil
Rabbit Glue Paraloid B72
Fig. 6. The maximum load at break point for the five adhesives applied on fir and maple samples after accelerating ageing with RH-T cycles. All values are average of four replicates.