PSI - Issue 47

Mikhail Sokovikov et al. / Procedia Structural Integrity 47 (2023) 693–697

696

4

Author name / Structural Integrity Procedia 00 (2019) 000–000

a

b

Fig.2. Structure of the examined specimen after tests in the split Hopkinson pressure bar; a - central part of the stress concentration zone; b- peripheral part of the stress concentration zone; a,b - longitudinal section; a - x6000; b - x8000

a

b

c

d

Fig.3. Temperature distribution in the examined AMg6 alloy specimen at different moments of time (from left to right and from top to bottom): a- 1∙10 -4 s, b - 2∙10 -4 s, c- 3∙10 -4 s, d - 4 ∙ 10 -4

Made with FlippingBook Digital Proposal Maker