A. Martín-Meizoso et alii, Frattura ed Integrità Strutturale, 30 (2014) 14-22; DOI: 10.3221/IGF-ESIS.30.03

Figure 6 : Necking and fracture of a mini-tensile probe.

1200

1200

1000

1000

800

800

600

600

400

400

200 Engineering STRESS (MPa)

Engineering STRESS (MPa)

200

0

-2000 -1500 -1000 -500 0

0 0.02 0.04 0.06 0.08 0.1 0.12 0.14 0.16 0.18 0.2 0

0.05 0.1 0.15 0.2

0

Mid-Distance from Flame cut (microns)

Engineering STRAIN

Engineering STRAIN

Figure 7 : Evolution of engineering stress vs. engineering strain as a function of distance from oxy-fuel cut edge, for the upper locations of cut edge (2.5 mm below upper plate surface).

1200

1200

1000

1000

800

800

600

600

400

400

200 Engineering STRESS (MPa)

Engineering STRESS (MPa)

200

0

-2000 -1500 -1000 -500 0

0 0.02 0.04 0.06 0.08 0.1 0.12 0.14 0.16 0.18 0.2 0

0.05 0.1 0.15 0.2

0

Mid-Distance from Flame cut (microns)

Engineering STRAIN

Engineering STRAIN

Figure 8 : Evolution of engineering stress vs. engineering strain as a function of distance from oxy-fuel cut edge, for middle thickness location of cut edge.