Crack Paths 2012
load, fatigue cracks begin to occur on AISI 304 stainless steel, which has the lowest
yield and fatigue strength values, in the distance of 16 m mafter welding point of E R
309L and AISI 304 stainless steels. If the construction is subjected to o=302.5 M P a
stress value, it can work 1,780,000 cycles properly. As for o=207 M P astress value,
which is under the yield strength value of the materials, it can work permanently.
Therefore, 107 cycles can be attributed as fatigue life of this construction for (5:207
M P a .
Acknowledgments
This study is supported by T U B I T A(KThe Scientific and Technological Research
Council of Turkey) under the Project Number106M091. The authors would also thank
to BahadirU Y U L G ATNevf,ikA K S OanYd JamesM A R R O W .
References
1- J.A.M. Pinho D a Cruz, J.D.M. Costa, L.F.P. Borrego, J.A.M. Ferreira, Fatigue
life prediction in AlMgSillap joint weldments, International Journal of Fatigue
22 (2000) 601-610.
940