Crack Paths 2006
1200
1000
800
[ N ] L O A D
600
400
200
Load- Experiment
Predicted load- upper bound
Predicted load - lower bound
A2/A1
0
0.0726
0.1726
0.2726
0.3726
0.4726
0.5726
0.6726
Figure 4: Critical load experimental and prediction for the P M M sApecimens.
Experiments on four-point bending specimens made of M A C O R
Four point bending (4PB) experiments were conducted on Machinable Ceramic
(MACOR- manufactured by Aremco) notched specimens at room temperature
(
E
] , [ 6 6 9 0 0 M P a c V
] , [ 1 0 3 IC
K M P a |
] [ 2 . 1 m M P a
) were loaded so to produce a
mixed mode loading state at the notch tip. In Figure 5 we show pictures of the crack
created at the V-notch tip in the various specimens.
Figure 5: Pictures of the crack at the
0 3 1 5 V-notch tip in 4PBM A C OsRpecimens
Made with FlippingBook Digital Publishing Software